Germany X2CrNiN1810
● Features and application:
Both the requirements for the manufacture of corrosion-resistant, but also requires a certain strength of structural components, such as food equipment, chemical equipment and nuclear industries.
● Chemical Composition:
Carbon C: ≤ 0.030
Si Si: ≤ 1.00
Manganese Mn: ≤ 2.00
Sulfur S: ≤ 0.030
Phosphorus P: ≤ 0.035
Chromium Cr: 17.00 ~ 19.00
Ni-Ni: 8.50 ~ 11.50
N N: 0.12 ~ 0.22
● Mechanical Properties:
Tensile strength σb (MPa): ≥ 550
Conditions yield strength σ0.2 (MPa): ≥ 245
Elongation δ5 (%): ≥ 40
Reduction of area ψ (%): ≥ 50
Hardness: ≤ 217HB; ≤ 95HRB; ≤ 220HV
● Heat treatment and microstructure specifications:
Standard heat treatment: solution 1010 ~ 1150 ℃ fast-cooling.
Microstructure: Organizing for the austenitic type.
● Delivery status:
Generally heat treatment delivery, the treatment types specified in the contract; not indicated, according to the heat treatment state of delivery.